{"id":5411,"date":"2026-11-26T12:00:19","date_gmt":"2026-11-26T04:00:19","guid":{"rendered":"https:\/\/www.oc-epc.com\/?p=5411"},"modified":"2026-11-27T18:12:03","modified_gmt":"2026-11-27T10:12:03","slug":"incomplete-eps-mold-filling-diagnosis","status":"publish","type":"post","link":"https:\/\/www.oc-epc.com\/vi\/news-blog\/industry-news\/incomplete-eps-mold-filling-diagnosis\/","title":{"rendered":"Incomplete EPS Mold Filling Diagnosis"},"content":{"rendered":"
<\/p>\n
Incomplete EPS mold filling should be diagnosed by location and repeatability before anyone raises feeding pressure. A defect that repeats beside one fill gun points toward a local gun, passage, or vent problem. A defect that moves between cycles suggests bead condition, supply stability, or recipe control. Separating those patterns prevents a filling fault from being hidden by a steam or fusion adjustment.<\/p>\n
A true short fill leaves part of the cavity without the intended bead mass. Missing rib tips, rounded incomplete corners, local voids, or a thin area that never packs can indicate a filling problem. Poor fusion is different: the cavity may be full, but the beads remain weakly bonded or visibly separate. Shrinkage and deformation occur later and require a different investigation.<\/p>\n
Mark the defect on a mold diagram and photograph the same orientation for several consecutive cycles. Record whether the location remains fixed, whether more than one cavity is affected, and whether the symptom began after a mold change, material change, cleaning activity, or utility disturbance. A single rejected pattern contains less information than a sequence with the same traceable references.<\/p>\n